2026/09/07
TPE Molding Case | How to Avoid Demolding Damage? 🔋🚗
This TPE part is a dust cover for a New Energy Vehicle (EV) charging port, where the customer requires a defect-free surface.
During production, the customer encountered demolding damage and ejector breakthrough.
🔍 Root Cause
The hot runner temperature was 250°C and injection temperature was 230°C. Combined with insufficient material drying, the TPE degraded and tended to stick to the mold, causing damage during ejection.
🔧 Our Solution
✔ Hot runner: 250°C → 210°C
✔ Injection temperature: 230°C → 200°C
✔ Drying: 90°C for 4 hours
After optimization, the demolding and surface quality were successfully improved.
For this application, our TPE provides:
✔ Good scratch resistance
✔ Easy molding
✔ Suitable for applications with high surface-quality requirements
Higher processing temperature is not always better. The right temperature and material preparation are key to a clean, defect-free TPE surface.